水泥穩(wěn)定碎石怎么取不出完整的芯樣?

來源:http://www.yinyudi.com/ 日期:2023-01-04
按照技術(shù)規(guī)范要求,濟(jì)南水泥穩(wěn)定碎石層齡期7d~10d,應(yīng)能取出完整的鉆件,可實際情況是部分路段因為松散,不能取出完整的芯樣。其原因是什么呢?
According to the requirements of the technical specifications, the Jinan cement stabilized macadam layer has an age of 7d~10d, and it should be able to take out complete drill pieces. However, the actual situation is that some sections cannot take out complete core samples because they are loose. What is the reason?
1)水泥用量偏少造成骨料之間膠結(jié)不好,達(dá)不到強(qiáng)度;
1) The cement consumption is too small, resulting in poor cementation between aggregates and failure to reach the strength;
2)沒有完全按照規(guī)范要求進(jìn)行養(yǎng)護(hù),按規(guī)范要求每一段碾壓完成并經(jīng)壓實度檢查合格后,應(yīng)立即養(yǎng)生,宜采用濕砂進(jìn)行養(yǎng)生,砂層厚度為7cm~10cm。也可采用瀝青乳液進(jìn)行養(yǎng)生,無述條件時,也可用灑水車結(jié)常灑水進(jìn)行養(yǎng)生。養(yǎng)生期不宜少于7天;
2) If the curing is not carried out in full accordance with the specification requirements, the curing shall be carried out immediately after the compaction of each section is completed according to the specification requirements and the compactness is checked to be qualified. It is better to use wet sand for curing. The thickness of the sand layer is 7cm~10cm. Asphalt lotion can also be used for curing. If there are no conditions mentioned above, the watering cart can also be used for curing. The curing period should not be less than 7 days;
3)水泥穩(wěn)定碎石層原材料級配不好;
3) The raw materials of cement stabilized macadam are poorly graded;
4)含水量不合適,以至于水泥不能在混合料中完全水化和水解,水泥對碎石的穩(wěn)定作用沒發(fā)揮,影響水泥穩(wěn)定碎石的強(qiáng)度;
4) The water content is not appropriate, so that the cement cannot be fully hydrated and hydrolyzed in the mixture, and the cement does not play a role in stabilizing the crushed stone, affecting the strength of cement stabilized crushed stone;
5)水泥選用不當(dāng),普通硅酸鹽水泥,礦渣硅酸鹽水泥和火山灰質(zhì)硅酸鹽水泥都可用水泥穩(wěn)定碎石,但應(yīng)選用初凝時間3h以上和終凝時間較長(宜在6h以上)。不宜使用快硬水泥,早強(qiáng)水泥以及已受潮變質(zhì)的水泥;
5) Improper cement selection. Ordinary Portland cement, slag Portland cement and pozzolanic Portland cement can be used to stabilize crushed stone, but the initial setting time shall be more than 3h and the final setting time shall be longer (preferably more than 6h). Fast hardening cement, early strength cement and cement that has been damped and deteriorated should not be used;
6)拌合得不均勻,且沒在佳含水量下充分壓實,以及施工碾壓時間拖的過長,破壞了已結(jié)硬的水泥膠凝,使其強(qiáng)度下降。
6) Uneven mixing, insufficient compaction under good water content, and too long construction rolling time destroy the hardened cement gel and reduce its strength.
濟(jì)南水泥穩(wěn)定碎石
預(yù)防措施:
Preventive measures:
1)原材料方面,每批水泥應(yīng)檢驗合格后,才能進(jìn)行使用;對于碎石,要符合級配要求,大料徑不要超過31.5mm,對于不合格的材料嚴(yán)禁進(jìn)入場地;
1) In terms of raw materials, each batch of cement can only be used after passing the inspection; Crushed stone shall meet the grading requirements, and the large material diameter shall not exceed 31.5mm. Unqualified materials shall not enter the site;
2)改進(jìn)拌合工藝,盡量避免離析的產(chǎn)生,施工人員要加強(qiáng)對水泥劑的控制,發(fā)現(xiàn)了問題要及時改進(jìn)與處理;
2) The mixing process shall be improved to avoid segregation as much as possible. The construction personnel shall strengthen the control of the cement agent, and timely improve and handle the problems found;
3)抖合的計量器具要在開工前送計量質(zhì)量檢測中心進(jìn)行檢定,以保證稱量的準(zhǔn)確無誤;
3) Shattered measuring instruments shall be sent to the Measurement Quality Inspection Center for verification before commencement to ensure the accuracy of weighing;
4)在運輸過程中要避免使用小型送料車,混合料要覆蓋,減少運輸途中水分的蒸發(fā)。
4) Small feeder trucks shall be avoided during transportation, and the mixture shall be covered to reduce evaporation of water during transportation.
水泥穩(wěn)定碎石基層這些質(zhì)量問題的出現(xiàn),就要求操作人員應(yīng)該對每道工序要嚴(yán)格控制,只有這樣才能保證水泥穩(wěn)定碎石層的質(zhì)量,避免病害的產(chǎn)生。更多相關(guān)內(nèi)容就來我們網(wǎng)站http://www.yinyudi.com咨詢了解吧!
The occurrence of these quality problems of cement stabilized macadam base requires operators to strictly control each process. Only in this way can the quality of cement stabilized macadam be guaranteed and the occurrence of diseases be avoided. More relevant content will come to our website http://www.yinyudi.com Ask and understand!